Location » Home » Grades > Superalloys > GH4761

GB GH4761 Details

GH4761

GB GH4761 Standard Download

Tags

GH4761 Application:Nickel-base superalloy
Category Type Grade Designations
Grades Superalloys GH4761 China - GB ,
Chemical composition(mass fraction)(wt.%)
Elements Min.(≥) Max.(≤) Similar Remarks
C 0.02 0.07
Cr 12.0 14.0
Mo 1.4 1.9
Ni 42.0 45.0
W 2.8 3.2
Al 1.4 1.85
Ti 3.15 3.65
B - 0.01
Ce - 0.03
Mechanical properties of grade GH4761
Proof strength
Rp0.2 (MPa)
Tensile strength
Rm (MPa)
Impact energy
KV (J)
Elongation at fracture
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
779 (≥) 157 (≥) 44 41 33 Solution and Aging, Annealing, Ausaging, Q+T,etc 144
Physical properties of grade GH4761
Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
Modulus of elasticity
kN/mm2
Expansion rate
861 (≥) 314 (≥) 33 41 34 Solution and Aging, Annealing, Ausaging, Q+T,etc 431
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
382 286 221
GH4761 Range of products
Product type Products Dimension Processes Deliver Status
Plates / Sheets Plates / Sheets 0.08-200mm(T)*W*L Forging, hot rolling and cold rolling Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Steel Bar Round Bar, Flat Bar, Square Bar Φ8-1200mm*L Forging, hot rolling and cold rolling, Cast Black, Rough Turning, Shot Blasting,
Coil / Strip Steel Coil /Steel Strip 0.03-16.0x1200mm Cold-Rolled & Hot-Rolled Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Pipes / Tubes Seamless Pipes/Tubes, Welded Pipes/Tubes OD:6-219mm x WT:0.5-20.0mm Hot extrusion, Cold Drawn, Welded Annealed, Solution and Aging, Q+T, ACID-WASHED
Cross Reference Table(Equivalent Grade)
Grade Standard Country Application
GH4761 GB China
Nickel-base superalloy